Impacts of melt holding temperature on properties of the aluminum–copper–cullet metal composite
DOI:
https://doi.org/10.70882/afd1vr92Keywords:
Aluminum Copper Cullet powder Holding time Density Hardness and grain sizeAbstract
The aluminum–copper–cullet (Al–Cu–CP) metal composite was fabricated at three differ
ent holding temperatures (800°C, 900°C, and 1,000°C, respectively) using the stir casting
method. The composite was fabricated from Al, Cu, and CP. The holding temperature
was varied in order to ascertain the optimum temperature for the fabrication of the
composite. The Al–Cu–CP metal composite fabricated was characterized by checking its
physical and mechanical properties in order to ascertain its potentials and application.
The Al–Cu–CP metal composite fabricated at 800°C exhibited the best properties as the
properties of the composite fabricated at 900°C and 1,000°C were relatively inferior.
Thus, 800°C is the optimum holding temperature for the fabrication of the Al–Cu–CP
metal composite using the stir casting method.
Downloads
Downloads
Published
Issue
Section
License
Copyright (c) 2026 Journal of Pure and Applied Sciences (Science Forum)

This work is licensed under a Creative Commons Attribution-NonCommercial-ShareAlike 4.0 International License.